Starting Point Formulation UCAR Latex 455
Low-Temperature Bake, Black Iron Oxide Primer
Formulation Suggestion LP-3791 |
|
Ingredients |
|
|
| Pigment Grind |
|
Water |
275.0
|
33.0
|
|
CELLOSIZE™ QP-4400 Hydroxyethyl Cellulose |
1.5
|
0.1
|
|
Dispersant(1) |
6.0
|
0.7
|
|
Ammonium Hydroxide, 28% Aqueous Solution |
4.0
|
0.4
|
|
Antifoam(2) |
1.0
|
0.1
|
|
Preservative(3) |
1.0
|
0.1
|
|
Black Iron Oxide(4) |
100.0
|
2.3
|
|
Talc(5) |
100.0
|
4.2
|
|
Corrosion Inhibitive Pigment(6) |
90.0
|
2.7
|
| Letdown |
|
UCAR™ Vehicle 455 |
350.0
|
39.3
|
|
Ammonium Hydroxide, 28% Aqueous Solution |
5.0
|
0.6
|
|
Water-Soluble Alkyd(7) |
50.0
|
5.7
|
|
Butyl CELLOSOLVE™ Solvent |
10.0
|
1.3
|
|
Drier(8) |
1.0
|
0.1
|
|
Drier(9) |
0.2
|
|
|
Drier(10) |
0.5
|
|
|
Water |
80.0
|
9.6
|
|
| Total: |
1075.2
|
100.0
|
|
Procedure
Charge the grind components into a mixer under agitation. Disperse in a high-speed mill and add the letdown ingredients under slow agitation.
| Paint Properties |
|
Pigment Volume Concentration, % |
31.0
|
|
Viscosity, #4 Ford cup, sec |
10.7
|
|
pH |
35-45
|
|
Weight per Gallon, lb |
7.5-8.0
|
|
Pigment/Binder Ratio |
1.5/1.0
|
|
Total Solids, % by Weight |
45.0
|
Application
Bake 5 to 10 minutes at 275°F
|