Starting Point Formulation

UCAR Latex 300

Interior Satin/Semigloss Formulation
Formulation Suggestion I-2281

Ingredients
Pounds
Gallons
Pigment Grind

Water

108.3
12.96

Potassium Tripolyphosphate (KTPP)

1.0
0.05

Tamol 731

5.0
0.54

TRITON™ Nonionic Surfactant CF-10

3.0
0.34

Drewplus L-475

2.0
0.26

Kathon LX (1.5%)

1.5
0.18

Sodium Carbonate

3.0
0.14

Ti-Pure R-900

220.0
6.60

Atomite

60.0
2.66

Water

83.3
10.00
Letdown

UCAR™ Latex 300

334.2
37.53

UCAR Latex 6030

137.1
15.57

Drewplus L-475

2.0
0.26

UCAR POLYPHOBE™ TR-116

2.3
0.26

UCAR POLYPHOBE TR-117

17.4
1.94

Water

89.2
10.71

Total:
1069.4
100.00


Paint Properties

Pigment Volume Concentration, %

26.3

Volume Solids, %

36.7

Weight Solids, %

50.9

Weight per Gallon, lb

10.7

Stormer, KU

88 - 93

ICI, poise

1.3

pH, equilibrated

8.3 - 8.7

Heat-Aged Stability, 2 weeks @ 140°F, KU

+5

VOC, g/L

<5
Film Properties

Gloss, 60°

36

Contrast Ratio, 3 mil

0.975

Wet Adhesion, 500 cycles

Pass

Flow and Leveling, Leneta

9

Sag Resistance

8

NOTICE: No freedom from any patent owned by Seller or others is to be inferred. Because use conditions and applicable laws may differ from one location to another and may change with time, Customer is responsible for determining whether products and the information in this document are appropriate for Customer's use and for ensuring that Customer's workplace and disposal practices are in compliance with applicable laws and other governmental enactments. Seller assumes no obligation or liability for the information in this document. NO WARRANTIES ARE GIVEN; ALL IMPLIED WARRANTIES OF MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE ARE EXPRESSLY EXCLUDED.